Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

LOCTITE EA 9309.3

Main features

  • Glass-Bead Bondline Control
  • 34.5 MPa Aluminum Lap Shear
  • Lap Shear Was Evaluated After hot/wet

Product Description

LOCTITE EA 9309.3NA AERO is a toughened two-part epoxy paste adhesive for bonding metal skins and honeycomb core. The formulation contains 0.13 mm glass beads that help establish a controlled bondline during assembly. It produces flexible bonded joints and provides high shear and peel strength on prepared aluminum under the documented test configurations. The adhesive can cure at room temperature or with an elevated-temperature cycle, with a 35-minute pot life for a 450 g mixed mass at 25°C. Performance data include lap shear across -55°C to 82°C, peel testing, hot/wet exposure, water, hydraulic oil, fuel, anti-icing fluid, and salt spray.

Key features

  • Controlled bondline thickness: Integrated 0.13 mm glass beads help maintain the intended adhesive bondline.
  • Aluminum shear and peel performance: Typical ASTM D1002 lap shear at 25°C is 32.8-34.5 MPa, while T-peel reaches 214 N/25 mm under the stated aluminum preparation and cure conditions.
  • Room-temperature or heat cure: Cure for 3-5 days at 25°C or 1 hour at 82°C; pot life is 35 minutes for a 450 g mixed mass at 25°C.

Applications / Suitable for

  • Bonding aluminum metal skins to honeycomb core
  • Prepared aluminum joints requiring both shear and peel performance
  • Bonded assemblies evaluated for humidity, water, common fluid, and salt-spray exposure

Technical Specifications

General Properties
Color
The color
Pink-red (Part A) / Blue (Part B)
Mix Ratio
The amount of a constituent divided by the total amount of all other constituents in a mixture
100:22 by weight
Physical Properties
Viscosity (Part A)
150,000 to 300,000 mPa.s
Viscosity (Part B)
10 to 20 mPa.s

Additional Information

Adhesives | Two-part epoxy paste adhesive

LOCTITE EA 9309.3NA AERO

LOCTITE EA 9309.3NA AERO is a toughened, two-part epoxy paste adhesive for bonding metal skins and honeycomb core. Integrated 0.13 mm glass beads control bondline thickness, while the cured adhesive provides flexible joints with strong aluminum shear and peel performance. Test data cover low-temperature, ambient, elevated-temperature, hot/wet, fluid, water, and salt-spray conditions.

Toughened two-part epoxy paste 0.13 mm glass-bead bondline control High aluminum shear strength High aluminum peel strength Humidity and fluid resistance
LOCTITE EA 9309.3NA AERO two-part epoxy paste adhesive packaging

LOCTITE EA 9309.3NA AERO two-part epoxy paste adhesive.

As supplied

Component and material properties

Values apply to the separate, unmixed components unless otherwise stated. Viscosity values retain the stated instrument, spindle, speed, and temperature conditions.

Property Value Unit Method / condition
Product form Two-part toughened epoxy paste adhesive — Part A and Part B mixed immediately before application
Bondline control 0.13 mm Integrated 5 mil glass beads
Part A color Pink-red — As supplied
Part B color Blue — As supplied
Part A viscosity 150-300 Pa·s 25°C; Brookfield HBT, spindle 7 at 2.1 rad/s
Part B viscosity 0.01-0.02 Pa·s 25°C; Brookfield LVF, spindle 1 at 6.3 rad/s
Warranty life - Part A 1 year Stored below 25°C
Warranty life - Part B 1 year Stored below 25°C
Preparation and cure

Processing guidance

Prepare clean, dry bonding surfaces, mix the two components completely at the specified weight ratio, apply the adhesive, and maintain contact or pressure until the joint develops handling strength. Processing times and performance depend on mixed mass, temperature, surface preparation, bondline, and cure conditions.

Component conditioning: Bring the separate components close to room temperature, approximately 25°C, before mixing.
Mix ratio: Combine 100 parts Part A with 22 parts Part B by weight and mix thoroughly. Volume measurement is not recommended for structural applications unless special ratio-control precautions are used.
Pot life: 35 minutes for a 450 g mixed mass at 25°C, tested by ASTM D2471 in a water bath.
Batch-size limit: Do not mix quantities greater than 450 g. The reaction can generate excessive heat, uncontrolled decomposition, and toxic fumes.
Assembly: Apply to clean, dry, properly prepared surfaces and hold the parts in contact until the adhesive is set.
Handling strength: 12 hours at 25°C. Support tooling or cure pressure may then be removed, but full bond strength has not yet developed.
Cure: 3-5 days at 25°C or 1 hour at 82°C to achieve normal performance.
Storage and handling

Warranty life is 1 year for both components when stored below 25°C. Keep containers tightly closed in a cool, well-ventilated area away from incompatible materials. Part B has a safe storage range of 0-25°C and must not be heated above 100°C. This material is for industrial use only.

After cure

Cured mechanical and thermal properties

Typical bulk-resin data apply to the stated casting geometry, cure, conditioning, and test method. They are not bonded-joint design allowables.

Property Value Unit Method / condition
Tensile strength 32.2 MPa ASTM D638; 3.18 mm casting; cure 72 hours at 25°C; tested at 25°C
Tensile modulus 2,303 MPa ASTM D638; 3.18 mm casting; cure 72 hours at 25°C; tested at 25°C
Shear modulus 841 MPa Cure 72 hours at 25°C; tested at 25°C
Poisson's ratio 0.36 — Cure 72 hours at 25°C; tested at 25°C
Elongation at break 10 % ASTM D638; cure 72 hours at 25°C; tested at 25°C
Shore D hardness 80 — ASTM D2240; cure 72 hours at 25°C; tested at 25°C
Compressive strength 51.7 MPa ASTM D695; 12.7 mm casting; tested at 25°C
Compressive modulus 1,688 MPa ASTM D695; 12.7 mm casting; tested at 25°C
Glass transition temperature, dry 61 °C DMTA; cure 72 hours at 25°C
Glass transition temperature, wet 64 °C DMTA; cure 72 hours at 25°C; conditioned at 71°C and 85% RH to saturation
Glass transition temperature, dry 81 °C DMTA; cure 1 hour at 82°C
Glass transition temperature, wet 64 °C DMTA; cure 1 hour at 82°C; conditioned at 71°C and 85% RH to saturation

Cured electrical properties

Values describe bulk cured material. Electrical performance in an assembled joint depends on bondline, geometry, electrodes, conditioning, and operating conditions.

Property Value Unit Method / condition
Dielectric constant 4.33 / 4.29 / 4.17 — ASTM D150 at 0.1 / 1.0 / 10.0 kHz
Dissipation factor 0.018 / 0.014 / 0.028 — ASTM D150 at 0.1 / 1.0 / 10.0 kHz
Volume resistivity 1.36 × 1014 ohm·cm Bulk cured material
Surface resistivity 4.94 × 1014 ohm Bulk cured material
Thermal conductivity 4.50 × 10-4 cal/(s·cm·°C) Bulk cured material

Performance evidence

The following typical results are configuration-specific. Aluminum alloy, surface preparation, adherend thickness, cure, pressure or vacuum, conditioning, and test temperature materially affect the values.

Aluminum lap shear across test temperatures
  • 2024-T3 clad aluminum with FPL preparation, cured 72 hours at 25°C under 0.7 bar pressure: 37.7 MPa at -55°C, 32.8 MPa at 25°C, and 6.4 MPa at 82°C.
  • 2024-T3 bare aluminum with PAA preparation, cured 2 hours at 66°C under 0.7 bar pressure: 34.5 MPa at 25°C and 6.9 MPa at 82°C.
ASTM D1002; 1.6 mm aluminum adherends. The sub-ambient specimens were soaked for 30 minutes before testing.
Environmental exposure performance
After a 5-day cure at 25°C, PAA-treated 2024-T3 Alclad specimens produced typical lap shear values of 29.6-35.2 MPa when tested at 25°C after the specified hydraulic-oil, fuel, anti-icing-fluid, hydrocarbon, water, hot/wet, and salt-spray exposures. The unconditioned control measured 33.1 MPa.
ASTM D1002; 1.6 mm aluminum adherends with PAA preparation. Exposure duration and temperature varied by medium, from 7 days at 25°C to 30 days under water, hot/wet, or salt-spray conditions.
T-peel and floating roller peel
  • Typical T-peel at 25°C: 214 N/25 mm for 2024-T3 clad aluminum after a 72-hour cure at 25°C, and 142 N/25 mm for 2024-T3 bare aluminum after a 2-hour cure at 82°C.
  • Typical T-peel at -55°C: 138 N/25 mm and 93 N/25 mm for the same respective configurations.
  • Typical floating roller peel at 25°C: 418 N/25 mm on PAA-treated 2024-T3 bare aluminum after a 72-hour cure at 25°C.
T-peel per ASTM D1876 and floating roller peel per ASTM D3167. Specimen thickness, aluminum condition, PAA preparation, cure, and vacuum are configuration-specific.
Service-temperature definition and creep result
Approximate service temperature is 82°C, defined as the temperature at which the adhesive retains 6.9 MPa lap shear by ASTM D1002. Creep deflection was 0.0142 mm after 192 hours under an 11.0 MPa load at 25°C.
The service-temperature value is a test-defined threshold, not a statement that every bonded assembly retains unchanged properties to 82°C.
Application and evaluation contexts

Applications

Application fit depends on the exact aluminum alloy or facing, core construction, surface preparation, bondline, cure process, joint geometry, loads, and operating environment.

Aluminum skin bonded to honeycomb core with a controlled epoxy bondline
Metal skin-to-honeycomb core bonding
The paste form and integrated 0.13 mm glass beads support controlled adhesive placement between prepared metal skins and honeycomb core. The documented strength and peel data are based on prepared aluminum configurations.
Prepared aluminum overlap joint bonded with two-part epoxy paste adhesive
Prepared aluminum structural joints
Suitable for evaluation where prepared aluminum joints require both lap-shear and peel performance. Surface preparation, adherend condition, cure, pressure or vacuum, and joint design must follow the application-specific process.
Bonded aluminum assembly exposed to humidity, water, fluids, and salt spray
Environmentally exposed bonded assemblies
The adhesive may be evaluated for prepared aluminum assemblies exposed to humidity, water, hydraulic oil, fuel, anti-icing fluid, hydrocarbon fluids, or salt spray. Exposure results apply only to the stated specimens, cure, conditioning, and test method.
Next steps

Evaluate LOCTITE EA 9309.3NA AERO for your bonded assembly

Contact Krayden to discuss aluminum or honeycomb-core substrates, surface preparation, bondline control, mix and cure conditions, test requirements, samples, and commercial availability for your application.

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers