EPOCAST 1627-2

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

EPOCAST 1627-2

Main features

  • Low-Thermal-Expansion Epoxy Syntactic
  • Composite-Core Reinforcement Compound
  • BMS 5-21 Type 2 Qualification

Product Description

EPOCAST® 1627-2 is a one-part, filled epoxy syntactic compound for fabricating and reinforcing composite structures. Supplied frozen as gray patties or in Semco cartridges, it is ready to apply after thawing and requires no weighing or mixing. The cured material combines a typical compressive strength of 30.0 ksi (207 MPa) at 77°F (25°C) with a low coefficient of thermal expansion of 11.2 × 10⁻⁶ in/in/°F (20.2 × 10⁻⁶ in/in/°C). Multiple heat-cure options support processing flexibility, and the product is qualified to BMS 5-21, Type 2.

Key features

  • Ready-to-use one-part format: Applies after thawing without component weighing or mixing.
  • High compressive strength: Provides a typical cured compressive strength of 30.0 ksi (207 MPa) at 77°F (25°C).
  • Low thermal expansion: Features a typical coefficient of thermal expansion of 11.2 × 10⁻⁶ in/in/°F (20.2 × 10⁻⁶ in/in/°C).

Technical Specifications

General Properties
Color
The color
Gray
Density (g)
1.8 g/cm3
Work life @25°C
Work life is the amount of time we have to work with a material until it is no longer able to be easily worked and applied on a substrate. It is based on the change in viscosity and it can rely on the application requirements.
24 hours

Additional Information

Technical properties

As-supplied / before-processing properties

Values shown are typical unless otherwise noted. Cure temperature refers to the actual material temperature measured by thermocouple.

Property Value Unit Method / condition
Appearance Gray — Visual; as supplied
Density 1.8 g/cm³ ASTM D1622
Extrudability 1,000 g/min BMS 5-28; at 77°F (25°C)
Work life 24 hours At 77°F (25°C)
Thaw time 1.5–2 hours At room temperature in the original sealed bag; protect from condensing humidity
Typical cure cycles 1 hour at 350°F (177°C)
6 hours at 250°F (121°C)
3–4 days at 180°F (83°C)
— Material temperature; heat and cool at 5–7°F (3–4°C) per minute, cooling to 150°F (66°C) or below
Technical properties

After-processing / final-state properties

The following cured-material results are typical values and do not constitute guaranteed product specifications.

Property Value Unit Method / condition
Compressive strength 30.0 (207) ksi (MPa) ASTM D695; at 77°F (25°C)
Compressive strength 3.5 (24) ksi (MPa) ASTM D695; at 325°F (163°C)
Compressive modulus 1,900 (13,100) ksi (MPa) ASTM D695; at 77°F (25°C)
Compressive modulus 60.0 (414) ksi (MPa) ASTM D695; at 325°F (163°C)
Shrinkage 0.002 in/in ASTM D696
Coefficient of thermal expansion 11.2 × 10⁻⁶ (20.2 × 10⁻⁶) in/in/°F (in/in/°C) ASTM D3386
Tensile lap shear strength 1,000 (6.9) psi (MPa) ASTM D1002; aluminum-to-aluminum at 77°F (25°C)
Tensile lap shear strength 500 (3.4) psi (MPa) ASTM D1002; aluminum-to-aluminum at 325°F (163°C)