COOLTHERM PC10882

Harmonization Code : 3910.00.00.90 | Silicones in Primary Forms; Others

COOLTHERM PC10882

Main features

  • Screen-Printable Coating Application
  • Thermal-Shock and Solvent-Resistant Cured Film
  • Above 500 V/mil Dielectric Strength

Product Description

LORD® PC10882 Protective Coating is a mineral-filled epoxy dielectric paste designed for screen printing as a protective coating over trimmed resistors and for general circuit protection. The dark-blue paste has a typical 65–85 kcP viscosity at 25°C and can be applied through 100–250 mesh stainless-steel screens with organic-emulsion backing. After printing, allow the coating to level for 5–10 minutes at room temperature, oven-dry for 5–10 minutes at 150°C to remove solvent, and use 245°C for 30 minutes as the documented cure guide. The cured film provides typical insulation resistance above 1 × 1011 ohm-cm at 2 mils, dielectric strength above 500 V/mil, a dielectric constant of 5–7, and dissipation factor below 1%.

Key features

  • Mineral-filled epoxy dielectric coating for printed circuit protection
  • Screen-printable through 100–250 mesh stainless-steel screens
  • Supports squeegee velocities up to 25 cm/s with a sharp 45° squeegee
  • Tough cured film positioned for thermal-shock, moisture, abrasion, oxidation, and solvent protection
  • Typical dielectric strength above 500 V/mil
  • LORD® 3996 thinner may be used when dilution is required
  • Six-month shelf life at 25°C in the original unopened container

Applications

  • Protective coating of trimmed resistors
  • General circuit protection
  • Screen-printed dielectric protection on validated substrates

Technical Specifications

General Properties
Appearance
Appearance at room temperature.
Dark Blue Paste
Physical Properties
Viscosity
Viscosity is a measurement of a fluid’s resistance to flow. Viscosity is commonly measured in centiPoise (cP). One cP is defined as the viscosity of water and all other viscosities are derived from this base. MPa is another common unit with a 1:1 conversion to cP. A product like honey would have a much higher viscosity -around 10,000 cPs- compared to water. As a result, honey would flow much slower out of a tipped glass than water would. The viscosity of a material can be decreased with an increase in temperature in order to better suit an application
65000-85000 mPa.s

Additional Information

Screen-printed dielectric surface protection

LORD® PC10882 Protective Coating

A mineral-filled epoxy dielectric paste designed for screen printing over trimmed resistors and for general circuit protection. The material forms a tough cured film that combines electrical insulation with documented resistance positioning against thermal shock, moisture, abrasion, oxidation, and commonly used solvents.

Dark-blue epoxy paste 65–85 kcP 100–250 mesh printing 245°C cure guide >500 V/mil
LORD PC10882 dark-blue protective coating container

LORD PC10882 dark-blue protective coating container

As supplied

Printable dielectric-paste properties

PC10882 is supplied as a dark-blue paste. The technical datasheet and safety data sheet use different viscosity test descriptions, so each value remains tied to its source and method.

Property Typical value Context
Appearance Dark-blue paste Mineral-filled epoxy dielectric material.
Viscosity at 25°C 65–85 kcP TDS: Brookfield RVT, spindle 6, 10 rpm.
SDS dynamic viscosity ≥75,000 mPa·s at 25°C Safety-document value; do not substitute it for the TDS processing range.
Density 1.79 g/cm³ SDS physical-property value.
Flash point 73°C Pensky-Martens closed cup; combustible-liquid handling applies.
VOC, calculated 375 g/L SDS value; regulatory interpretation is jurisdiction-dependent.
Application process

Gently mix, screen print, level, remove solvent, and complete the high-temperature cure

Gently stir the material before use. When dilution is needed, use LORD® 3996 Thinner. Apply by screen printing through 100–250 mesh stainless-steel screens with organic-emulsion backing.

  • Use a sharp squeegee with a 45° angle of attack.
  • The documented maximum squeegee velocity is 25 cm/s.
  • Allow the printed material to self-level for 5–10 minutes at room temperature.
  • Oven-dry for 5–10 minutes at 150°C to remove solvent.
  • Cure at 245°C for 30 minutes as the published guide.
  • Determine the optimum cure empirically for the actual substrate, print thickness, oven, fixture, and part geometry.
MIXPAC™ MixCoat™ Flex Protective Coating Dispensing System forLORD PC10882

Insert a process visual showing gentle stirring, optional LORD® 3996 thinning, 100–250 mesh screen printing, 5–10 minute levelling, 150°C solvent drying, and 245°C cure.

1. Condition material

Gently stir and add only the documented thinner when dilution is required.

2. Screen print

Use the specified stainless-steel mesh, emulsion backing, sharp squeegee, and controlled velocity.

3. Level and dry

Level at room temperature, then remove solvent at 150°C.

4. Cure and validate

Use 245°C for 30 minutes as a guide and validate the final production cycle.

Storage and industrial handling

Shelf life is six months from the date of shipment when stored at 25°C in the original unopened container. Keep the container tightly closed, upright, cool, and in a well-ventilated area away from heat, sparks, open flames, and strong acids, bases, or oxidisers. The current SDS classifies PC10882 as a combustible liquid and identifies serious eye, chronic-health, organ-toxicity, and aquatic hazards. Use only in trained industrial or commercial operations with the ventilation, respiratory, skin, eye, hygiene, ignition-control, spill, and waste measures required by the current regional SDS and workplace assessment.

Final cured film

Dielectric and electrical properties

These values are typical cured-film results. Insulation resistance is reported at a 2 mil film thickness; dielectric strength is not a guaranteed working voltage for a finished circuit or component.

Property Typical value Context
Insulation resistance >1 × 1011 ohm-cm Reported at 2 mils cured-film thickness.
Dielectric strength >500 V/mil Typical breakdown property; not a finished-device working-voltage rating.
Dielectric constant 5–7 Frequency and conditioning are not stated in DS3826.
Dissipation factor <1% Frequency and conditioning are not stated in DS3826.
Applications and protection

Printed protection for resistors and electronic circuits

PC10882 is directly designed for protective coating of trimmed resistors and for general circuit protection. Its cured-film protection statements apply only after the coating has been printed, levelled, solvent-dried, fully cured, and validated on the actual substrate and film geometry.

Trimmed resistor covered with screen-printed dielectric protective coating

Trimmed-resistor protection

Designed to form a printed dielectric protective layer over trimmed resistor areas.

Electronic circuit area protected with a dark-blue screen-printed epoxy coating

General circuit protection

May be evaluated as a printed dielectric coating for circuit areas requiring the documented cured-film properties.

Cured epoxy dielectric coating exposed to moisture abrasion oxidation and thermal cycling

Environmental surface protection

The fully cured film is positioned for protection against thermal shock, moisture, abrasion, oxidation, and many commonly used solvents.

Validate PC10882 for your screen-printing and circuit-protection process

Krayden can help review substrate preparation, mesh and emulsion selection, squeegee geometry and velocity, dilution, wet-film deposition, levelling, solvent removal, cure profile, final thickness, electrical insulation, environmental exposure, and production qualification for LORD® PC10882.

Contact Krayden Technical Support

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers